Whilst we try to ensure that this table is as accurate as possible we cannot guarantee that the data contained in the tables is accurate for all blends and grades of PVC. This is particularly so for plasticised PVC where the plasticiser used will affect the chemical resistance of the compound. In all cases the supplier of the compound should be contacted to determine the exact chemical resistance of the material.


PVC-plasticised

A B C D E F G H I L M N O P S T U V W Y Z

 R = Resistant

LR = Limited Resistance

NR = Not Recommended

ND = No Data

Chemical

Resistance

20oC 60oC 100oC
Acetaldehyde NR NR ND
Acetic acid (10%) R NR ND
Acetic acid (glac./anh.) NR NR ND
Acetic anhydride NR NR ND
Aceto-acetic ester ND ND ND
Acetone NR NR ND
Other ketones NR NR ND
Acetonitrile NR NR ND
Acetylene ND ND ND
Acetyl salicylic acid ND ND ND
Acid fumes ND ND ND
Alcohols ND ND ND
Aliphatic esters ND ND ND
Alkyl chlorides ND ND ND
Alum R R ND
Aluminium chloride R R ND
Aluminium sulphate R R ND
Ammonia, anhydrous NR NR ND
Ammonia, aqueous ND ND ND
Ammonium chloride R R ND
Amyl acetate NR NR ND
Aniline NR NR ND
Antimony trichloride R R ND
Aqua regia ND ND ND
Aromatic solvents ND ND ND
Ascorbic acid ND ND ND
Beer R NR ND
Benzaldehyde NR NR ND
Benzene NR NR ND
Benzoic acid ND NR ND
Benzoyl peroxide ND ND ND
Boric acid R NR ND
Brines, saturated R R ND
Bromide (K) solution R R ND
Bromine NR NR ND
Bromine liquid, tech. NR NR ND
Bromine water, saturated aqueous NR NR ND
Butyl acetate NR NR ND
Calcium chloride R R ND
Carbon disulphide NR NR ND
Carbonic acid R R ND
Carbon tetrachloride NR NR ND
Caustic soda & potash R NR ND
Cellulose paint ND ND ND
Chlorates of Na, K, Ba ND ND ND
Chlorine, dry ND ND ND
Chlorine, wet ND ND ND
Chlorides of Na, K, Ba R R ND
Chloroacetic acid NR NR ND
Chlorobenzene NR NR ND
Chloroform NR NR ND
Chlorosulphonic acid NR NR ND
Chromic acid (80%) NR NR ND
Citric acid R NR ND
Copper salts (most) R R ND
Cresylic acids (50%) NR NR ND
Cyclohexane ND ND ND
Detergents, synthetic R NR ND
Emulsifiers, concentrated R R ND
Esters NR NR ND
Ether ND ND ND
Fatty acids (>C6) ND ND ND
Ferric chloride R R ND
Ferrous sulphate R R ND
Fluorinated refrigerants NR NR ND
Fluorine, dry NR NR ND
Fluorine, wet NR NR ND
Fluorosilic acid ND ND ND
Formaldehyde (40%) R NR ND
Formic acid ND ND ND
Fruit juices R R ND
Gelatine ND ND ND
Glycerine R NR ND
Glycols ND ND ND
Glycol, ethylene R R ND
Glycolic acid ND ND ND
Hexamethylene diamine ND ND ND
Hexamine ND ND ND
Hydrazine ND ND ND
Hydrobromic acid (50%) R R ND
Hydrochloric acid (10%) R R ND
Hydrochloric acid (conc.) R LR ND
Hydrocyanic acid ND ND ND
Hydrofluoric acid (40%) R NR ND
Hydrofluoric acid (75%) NR NR ND
Hydrogen peroxide (30%) R NR ND
Hydrogen peroxide (30 - 90%) R NR ND
Hydrogen sulphide R NR ND
Hypochlorites R LR ND
Hypochlorites (Na 12-14%) R R ND
Iso-butyl-acetate ND ND ND
Lactic acid (90%) NR NR ND
Lead acetate R R ND
Lead perchlorate ND ND ND
Lime (CaO) R ND ND
Maleic acid NR NR ND
Manganate, potassium (K) R R ND
Meat juices ND ND ND
Mercuric chloride NR NR ND
Mercury R R ND
Methanol R R ND
Methylene chloride NR NR ND
Milk products R NR ND
Moist air R R ND
Molasses R R ND
Monoethanolamine ND ND ND
Naptha ND ND ND
Napthalene NR NR ND
Nickel salts R R ND
Nitrates of Na, K and NH3 R R ND
Nitric acid (<25%) R ND ND
Nitric acid (50%) R ND ND
Nitric acid (90%) NR NR ND
Nitric acid (fuming) NR NR ND
Nitrite (Na) NR NR ND
Nitrobenzene NR NR ND
Oils, diesel ND ND ND
Oils, essential ND ND ND
Oils, lubricating + aromatic additives ND ND ND
Oils, mineral R NR ND
Oils, vegetable and animal R ND ND
Oxalic acid R NR ND
Ozone R NR ND
Paraffin wax ND ND ND
Perchloric acid ND NR ND
Petroleum spirits R NR ND
Phenol ND NR ND
Phosphoric acid (20%) R R ND
Phosphoric acid (50%) ND ND ND
Phosphoric acid (95%) ND ND ND
Phosphorous chlorides ND ND ND
Phosphorous pentoxide R ND ND
Phthalic acid NR NR ND
Picric acid R ND ND
Pyridine ND ND ND
Salicyl aldehyde ND ND ND
Sea water R R ND
Silicic acid ND ND ND
Silicone fluids ND ND ND
Silver nitrate R R ND
Sodium carbonate R ND ND
Sodium peroxide R R ND
Sodium silicate R R ND
Sodium sulphide R R ND
Stannic chloride R R ND
Starch R R ND
Sugar, syrups & jams ND ND ND
Sulphamic acid ND ND ND
Sulphates (Na, K, Mg, Ca) ND ND ND
Sulphites ND ND ND
Sulphonic acids ND ND ND
Sulphur ND ND ND
Sulphur dioxide, dry R NR ND
Sulphur dioxide, wet R R ND
Sulphur dioxide (96%) R R ND
Sulphur trioxide ND ND ND
Sulphuric acid (<50%) R LR ND
Sulphuric acid (70%) LR ND ND
Sulphuric acid (95%) ND ND ND
Sulphuric acid, fuming NR NR ND
Sulphur chlorides ND ND ND
Tallow R ND ND
Tannic acid (10%) R ND ND
Tartaric acid R ND ND
Trichlorethylene NR NR ND
Urea (30%) R R ND
Vinegar R ND ND
Water, distilled R R ND
Water, soft R R ND
Water, hard R R ND
Wetting agents (<5%) R R ND
Yeast R ND ND
Zinc chloride R R ND

 