PP

A B C D E F G H I L M N O P S T U V W Y Z

R = Resistant

LR = Limited Resistance

NR = Not Recommended

ND = No Data 

Chemical

Resistance

20oC 60oC 100oC
Acetaldehyde R ND NR
Acetic acid (10%) R R ND
Acetic acid (glac./anh.) R R NR
Acetic anhydride R R NR
Aceto-acetic ester R R R
Acetone R R ND
Other ketones R NR NR
Acetonitrile R R ND
Acetylene ND ND ND
Acetyl salicylic acid LR LR LR
Acid fumes R R NR
Alcohols R R ND
Aliphatic esters R NR NR
Alkyl chlorides NR NR NR
Alum R R R
Aluminium chloride R R R
Aluminium sulphate R R R
Ammonia, anhydrous R R R
Ammonia, aqueous R R R
Ammonium chloride R R R
Amyl acetate R NR NR
Aniline R R R
Antimony trichloride R R ND
Aqua regia R NR NR
Aromatic solvents R NR NR
Ascorbic acid ND ND ND
Beer R R ND
Benzaldehyde R R NR
Benzene NR NR NR
Benzoic acid R R ND
Benzoyl peroxide NR NR NR
Boric acid R R R
Brines, saturated R R ND
Bromide (K) solution R R ND
Bromine NR NR NR
Bromine liquid, tech. ND ND ND
Bromine water, saturated aqueous ND ND ND
Butyl acetate R NR NR
Calcium chloride R R R
Carbon disulphide NR NR NR
Carbonic acid R R ND
Carbon tetrachloride NR NR NR
Caustic soda & potash R R R
Cellulose paint NR NR NR
Chlorates of Na, K, Ba R R ND
Chlorine, dry NR NR NR
Chlorine, wet NR NR NR
Chlorides of Na, K, Ba R R R
Chloroacetic acid R R ND
Chlorobenzene NR NR NR
Chloroform NR NR NR
Chlorosulphonic acid NR NR NR
Chromic acid (80%) R ND ND
Citric acid R R ND
Copper salts (most) R R ND
Cresylic acids (50%) ND ND ND
Cyclohexane NR NR NR
Detergents, synthetic R R R
Emulsifiers, concentrated R R ND
Esters R NR NR
Ether NR NR NR
Fatty acids (>C6) R R ND
Ferric chloride R R R
Ferrous sulphate R R R
Fluorinated refrigerants NR NR NR
Fluorine, dry NR NR NR
Flourine, wet NR NR NR
Fluorosilic acid R R ND
Formaldehyde (40%) R R ND
Formic acid R ND ND
Fruit juices R R ND
Gelatine R R ND
Glycerine R R R
Glycols R R ND
Glycol, ethylene R R R
Glycolic acid R R R
Hexamethylene diamine NR NR NR
Hexamine ND ND ND
Hydrazine R ND ND
Hydrobromic acid (50%) R R R
Hydrochloric acid (10%) R R R
Hydrochloric acid (conc.) R R NR
Hydrocyanic acid R R ND
Hydrofluoric acid (40%) R ND ND
Hydrofluoric acid (75%) R ND NR
Hydrogen peroxide (30%) NR NR NR
Hydrogen peroxide (30 - 90%) NR NR NR
Hydrogen sulphide R R ND
Hypochlorites R R R
Hypochlorites (Na 12-14%) R R R
Iso-butyl-acetate R NR NR
Lactic acid (90%) R R ND
Lead acetate R R ND
Lead perchlorate NR NR NR
Lime (CaO) R R R
Maleic acid R R R
Manganate, potassium (K) R R ND
Meat juices R R ND
Mercuric chloride R R ND
Mercury R R R
Methanol R R R
Methylene chloride NR NR NR
Milk products R R R
Moist air R R R
Molasses R R ND
Monoethanolamine LR LR LR
Naptha R ND ND
Napthalene R R R
Nickel salts R R R
Nitrates of Na, K and NH3 R R ND
Nitric acid (<25%) R R R
Nitric acid (50%) NR NR NR
Nitric acid (90%) NR NR NR
Nitric acid (fuming) NR NR NR
Nitrite (Na) NR NR NR
Nitrobenzene LR LR LR
Oils, diesel R NR NR
Oils, essential R R R
Oils, lubricating + aromatic additives R NR NR
Oils, mineral R NR NR
Oils, vegetable and animal R R NR
Oxalic acid R R NR
Ozone ND ND ND
Paraffin wax R R ND
Perchloric acid NR NR NR
Petroleum spirits NR NR NR
Phenol R R ND
Phosphoric acid (20%) R R R
Phosphoric acid (50%) R R ND
Phosphoric acid (95%) R R ND
Phosphorous chlorides R ND ND
Phosphorous pentoxide R R ND
Phthalic acid R R ND
Picric acid R R ND
Pyridine R ND ND
Salicyl aldehyde ND ND ND
Sea water R R R
Silicic acid R R ND
Silicone fluids R R ND
Silver nitrate R R ND
Sodium carbonate R R ND
Sodium peroxide ND ND ND
Sodium silicate R R R
Sodium sulphide R R R
Stannic chloride R R R
Starch R R R
Sugar, syrups & jams R R ND
Sulphamic acid R R ND
Sulphates (Na, K, Mg, Ca) R R NR
Sulphites R R ND
Sulphonic acids ND ND ND
Sulphur R R ND
Sulphur dioxide, dry R R NR
Sulphur dioxide, wet R R ND
Sulphur dioxide (96%) R R ND
Sulphur trioxide ND ND ND
Sulphuric acid (<50%) R R NR
Sulphuric acid (70%) R NR NR
Sulphuric acid (95%) R NR NR
Sulphuric acid, fuming NR NR NR
Sulphur chlorides ND ND ND
Tallow R R ND
Tannic acid (10%) R R ND
Tartaric acid R R ND
Trichlorethylene NR NR NR
Urea (30%) R R NR
Vinegar R R ND
Water, distilled. R R R
Water, soft R R R
Water, hard R R R
Wetting agents (<5%) R R R
Yeast R R ND
Zinc chloride R R ND

 