Chemical |
Resistance |
|
20oC |
60oC |
100oC |
| Acetaldehyde |
R |
ND |
ND |
| Acetic
acid (10%) |
R |
ND |
ND |
| Acetic
acid (glac./anh.) |
LR |
ND |
ND |
| Acetic
anhydride |
LR |
ND |
ND |
| Aceto-acetic
ester |
ND |
ND |
ND |
| Acetone |
R |
ND |
ND |
| Other
ketones |
LR |
ND |
ND |
| Acetonitrile |
ND |
ND |
ND |
| Acetylene |
R |
ND |
ND |
| Acetyl
salicylic acid |
ND |
ND |
ND |
| Acid
fumes |
ND |
ND |
ND |
| Alcohols |
R |
ND |
ND |
| Aliphatic
esters |
R |
ND |
ND |
| Alkyl
chlorides |
R |
ND |
ND |
| Alum |
LR |
ND |
ND |
| Aluminium
chloride |
LR |
ND |
ND |
| Aluminium
sulphate |
LR |
ND |
ND |
| Ammonia,
anhydrous |
R |
ND |
ND |
| Ammonia,
aqueous |
R |
ND |
ND |
| Ammonium
chloride |
R |
ND |
ND |
| Amyl
acetate |
R |
ND |
ND |
| Aniline |
LR |
ND |
ND |
| Antimony
trichloride |
ND |
ND |
ND |
| Aqua
regia |
NR |
NR |
ND |
| Aromatic
solvents |
R |
ND |
ND |
| Ascorbic
acid |
ND |
ND |
ND |
| Beer |
R |
ND |
ND |
| Benzaldehyde |
ND |
ND |
ND |
| Benzene |
R |
ND |
ND |
| Benzoic
acid |
LR |
ND |
ND |
| Benzoyl
peroxide |
ND |
ND |
ND |
| Boric
acid |
LR |
ND |
ND |
| Brines,
saturated |
R |
ND |
ND |
| Bromide
(K) solution |
LR |
ND |
ND |
| Bromine |
NR |
NR |
ND |
| Bromine
liquid, tech. |
NR |
NR |
ND |
| Bromine
water, saturated aqueous |
NR |
NR |
ND |
| Butyl
acetate |
ND |
ND |
ND |
| Calcium
chloride |
R |
ND |
ND |
| Carbon
disulphide |
ND |
ND |
ND |
| Carbonic
acid |
ND |
ND |
ND |
| Carbon
tetrachloride |
R |
ND |
ND |
| Caustic
soda & potash |
R |
R |
ND |
| Cellulose
paint |
ND |
ND |
ND |
| Chlorates
of Na, K, Ba |
ND |
ND |
ND |
| Chlorine,
dry |
NR |
NR |
ND |
| Chlorine,
wet |
NR |
NR |
ND |
| Chlorides
of Na, K, Ba |
R |
R |
ND |
| Chloroacetic
acid |
NR |
NR |
ND |
| Chlorobenzene |
ND |
ND |
ND |
| Chloroform |
R |
ND |
ND |
| Chlorosulphonic
acid |
ND |
ND |
ND |
| Chromic
acid (80%) |
NR |
NR |
ND |
| Citric
acid |
LR |
ND |
ND |
| Copper
salts (most) |
R |
ND |
ND |
| Cresylic
acids (50%) |
ND |
ND |
ND |
| Cyclohexane |
R |
ND |
ND |
| Detergents,
synthetic |
R |
ND |
ND |
| Emulsifiers,
concentrated |
ND |
ND |
ND |
| Esters |
ND |
ND |
ND |
| Ether |
R |
R |
ND |
| Fatty
acids (>C6) |
R |
ND |
ND |
| Ferric
chloride |
LR |
ND |
ND |
| Ferrous
sulphate |
R |
ND |
ND |
| Fluorinated
refrigerants |
R |
ND |
ND |
| Fluorine,
dry |
ND |
ND |
ND |
| Flourine,
wet |
ND |
ND |
ND |
| Fluorosilic
acid |
ND |
ND |
ND |
| Formaldehyde
(40%) |
R |
ND |
ND |
| Formic
acid |
NR |
NR |
ND |
| Fruit
juices |
ND |
ND |
ND |
| Gelatine |
R |
ND |
ND |
| Glycerine |
R |
ND |
ND |
| Glycols |
ND |
ND |
ND |
| Glycol,
ethylene |
R |
ND |
ND |
| Glycolic
acid |
ND |
ND |
ND |
| Hexamethylene
diamine |
ND |
ND |
ND |
| Hexamine |
ND |
ND |
ND |
| Hydrazine |
ND |
ND |
ND |
| Hydrobromic
acid (50%) |
NR |
NR |
ND |
| Hydrochloric
acid (10%) |
NR |
NR |
ND |
| Hydrochloric
acid (conc.) |
NR |
NR |
ND |
| Hydrocyanic
acid |
ND |
ND |
ND |
| Hydrofluoric
acid (40%) |
NR |
NR |
ND |
| Hydrofluoric
acid (75%) |
R |
ND |
ND |
| Hydrogen
peroxide (30%) |
ND |
ND |
ND |
| Hydrogen
peroxide (30 - 90%) |
ND |
ND |
ND |
| Hydrogen
sulphide |
R |
ND |
ND |
| Hypochlorites |
LR |
ND |
ND |
| Hypochlorites
(Na 12-14%) |
NR |
NR |
ND |
| Iso-butyl-acetate |
ND |
ND |
ND |
| Lactic
acid (90%) |
LR |
ND |
ND |
| Lead
acetate |
R |
ND |
ND |
| Lead
perchlorate |
ND |
ND |
ND |
| Lime
(CaO) |
R |
ND |
ND |
| Maleic
acid |
ND |
ND |
ND |
| Manganate,
potassium (K) |
R |
ND |
ND |
| Meat
juices |
ND |
ND |
ND |
| Mercuric
chloride |
R |
ND |
ND |
| Mercury |
R |
ND |
ND |
| Methanol |
R |
ND |
ND |
| Methylene
chloride |
ND |
ND |
ND |
| Milk
products |
R |
ND |
ND |
| Moist
air |
R |
ND |
ND |
| Molasses |
R |
ND |
ND |
| Monoethanolamine |
ND |
ND |
ND |
| Naptha |
ND |
ND |
ND |
| Napthalene |
ND |
ND |
ND |
| Nickel
salts |
R |
ND |
ND |
| Nitrates
of Na, K and NH3 |
R |
ND |
ND |
| Nitric
acid (<25%) |
NR |
NR |
ND |
| Nitric
acid (50%) |
NR |
NR |
ND |
| Nitric
acid (90%) |
NR |
NR |
ND |
| Nitric
acid (fuming) |
NR |
NR |
ND |
| Nitrite
(Na) |
R |
ND |
ND |
| Nitrobenzene |
ND |
ND |
ND |
| Oils,
diesel |
R |
NR |
ND |
| Oils,
essential |
R |
R |
ND |
| Oils,
lubricating + aromatic additives |
R |
ND |
ND |
| Oils,
mineral |
ND |
ND |
ND |
| Oils,
vegetable and animal |
R |
ND |
ND |
| Oxalic
acid |
ND |
ND |
ND |
| Ozone |
ND |
ND |
ND |
| Paraffin
wax |
ND |
ND |
ND |
| Perchloric
acid |
R |
R |
ND |
| Petroleum
spirits |
ND |
ND |
ND |
| Phenol |
NR |
NR |
ND |
| Phosphoric
acid (20%) |
NR |
NR |
ND |
| Phosphoric
acid (50%) |
NR |
NR |
ND |
| Phosphoric
acid (95%) |
NR |
NR |
ND |
| Phosphorous
chlorides |
NR |
NR |
ND |
| Phosphorous
pentoxide |
NR |
NR |
ND |
| Phthalic
acid |
ND |
ND |
ND |
| Picric
acid |
LR |
ND |
ND |
| Pyridine |
LR |
ND |
ND |
| Salicyl
aldehyde |
ND |
ND |
ND |
| Sea
water |
R |
NR |
ND |
| Silicic
acid |
ND |
ND |
ND |
| Silicone
fluids |
ND |
ND |
ND |
| Silver
nitrate |
R |
NR |
ND |
| Sodium
carbonate |
R |
R |
ND |
| Sodium
peroxide |
ND |
ND |
ND |
| Sodium
silicate |
R |
ND |
ND |
| Sodium
sulphide |
R |
ND |
ND |
| Stannic
chloride |
ND |
ND |
ND |
| Starch |
R |
ND |
ND |
| Sugar,
syrups
& jams |
R |
ND |
ND |
| Sulphamic
acid |
LR |
ND |
ND |
| Sulphates
(Na, K, Mg, Ca) |
R |
ND |
ND |
| Sulphites |
R |
ND |
ND |
| Sulphonic
acids |
ND |
ND |
ND |
| Sulphur |
R |
ND |
ND |
| Sulphur
dioxide, dry |
LR |
ND |
ND |
| Sulphur
dioxide, wet |
LR |
ND |
ND |
| Sulphur
dioxide (96%) |
ND |
ND |
ND |
| Sulphur
trioxide |
ND |
ND |
ND |
| Sulphuric
acid (<50%) |
NR |
ND |
ND |
| Sulphuric
acid (70%) |
NR |
NR |
ND |
| Sulphuric
acid (95%) |
NR |
NR |
ND |
| Sulphuric
acid, fuming |
NR |
NR |
ND |
| Sulphur
chlorides |
LR |
ND |
ND |
| Tallow |
R |
ND |
ND |
| Tannic
acid (10%) |
LR |
ND |
ND |
| Tartaric
acid |
LR |
ND |
ND |
| Trichlorethylene |
LR |
ND |
ND |
| Urea
(30%) |
R |
ND |
ND |
| Vinegar |
LR |
ND |
ND |
| Water,
distilled. |
R |
ND |
ND |
| Water,
soft |
R |
ND |
ND |
| Water,
hard |
R |
ND |
ND |
| Wetting
agents (<5%) |
ND |
ND |
ND |
| Yeast |
ND |
ND |
ND |
| Zinc
chloride |
ND |
ND |
ND |