Chemical

Resistance

20oC 60oC 100oC
Acetaldehyde R R ND
Acetic acid (10%) R NR NR
Acetic acid (glac./anh.) NR NR NR
Acetic anhydride ND ND ND
Aceto-acetic ester ND ND ND
Acetone R R NR
Other ketones R ND ND
Acetonitrile ND ND ND
Acetylene ND ND ND
Acetyl salicylic acid ND ND ND
Acid fumes NR NR NR
Alcohols R R R
Aliphatic esters R ND NR
Alkyl chlorides R ND ND
Alum R R R
Aluminium chloride R ND ND
Aluminium sulphate R R R
Ammonia, anhydrous R ND ND
Ammonia, aqueous R ND ND
Ammonium chloride R ND ND
Amyl acetate R ND ND
Aniline R NR NR
Antimony trichloride ND ND NR
Aqua regia NR NR NR
Aromatic solvents R R R
Ascorbic acid ND ND ND
Beer R R R
Benzaldehyde ND NR NR
Benzene NR NR NR
Benzoic acid R NR NR
Benzoyl peroxide ND ND ND
Boric acid R R R
Brines, saturated R R R
Bromide (K) solution R ND ND
Bromine NR NR NR
Bromine liquid, tech. NR NR NR
Bromine water, saturated aqueous NR NR NR
Butyl acetate R ND ND
Calcium chloride ND ND NR
Carbon disulphide R ND ND
Carbonic acid R R ND
Carbon tetrachloride R ND ND
Caustic soda & potash R R R
Cellulose paint ND ND ND
Chlorates of Na, K, Ba R R ND
Chlorine, dry NR NR NR
Chlorine, wet NR NR NR
Chlorides of Na, K, Ba R R R
Chloroacetic acid NR NR NR
Chlorobenzene ND ND NR
Chloroform NR NR NR
Chlorosulphonic acid NR NR NR
Chromic acid (80%) NR NR NR
Citric acid ND ND NR
Copper salts (most) R R R
Cresylic acids (50%) NR NR NR
Cyclohexane R ND ND
Detergents, synthetic R R R
Emulsifiers, concentrated R R R
Esters R ND ND
Ether R ND ND
Fatty acids (>C6) R ND ND
Ferric chloride R NR NR
Ferrous sulphate R R R
Fluorinated refrigerants R ND ND
Fluorine, dry NR NR NR
Flourine, wet NR NR NR
Fluorosilic acid NR NR NR
Formaldehyde (40%) R R NR
Formic acid NR NR NR
Fruit juices R R R
Gelatine R R R
Glycerine R R ND
Glycols R R ND
Glycol, ethylene R R R
Glycolic acid NR NR NR
Hexamethylene diamine ND ND ND
Hexamine ND ND ND
Hydrazine ND ND ND
Hydrobromic acid (50%) NR NR NR
Hydrochloric acid (10%) NR NR NR
Hydrochloric acid (conc.) NR NR NR
Hydrocyanic acid NR NR NR
Hydrofluoric acid (40%) NR NR NR
Hydrofluoric acid (75%) NR NR NR
Hydrogen peroxide (30%) NR NR NR
Hydrogen peroxide (30 - 90%) NR NR NR
Hydrogen sulphide R ND ND
Hypochlorites NR NR NR
Hypochlorites (Na 12-14%) NR NR NR
Iso-butyl-acetate R ND ND
Lactic acid (90%) NR NR NR
Lead acetate R R ND
Lead perchlorate ND ND ND
Lime (CaO) R R ND
Maleic acid R ND ND
Manganate, potassium (K) NR NR NR
Meat juices R R R
Mercuric chloride R NR NR
Mercury R R R
Methanol R R R
Methylene chloride ND ND NR
Milk products R R R
Moist air R R R
Molasses R R R
Monoethanolamine ND ND ND
Naptha R ND ND
Napthalene R ND ND
Nickel salts ND ND ND
Nitrates of Na, K and NH3 R R ND
Nitric acid (<25%) NR NR NR
Nitric acid (50%) NR NR NR
Nitric acid (90%) NR NR NR
Nitric acid (fuming) NR NR NR
Nitrite (Na) NR NR NR
Nitrobenzene LR ND ND
Oils, diesel R R R
Oils, essential R R R
Oils, lubricating + aromatic additives R R R
Oils, mineral R R R
Oils, vegetable and animal R R R
Oxalic acid R ND ND
Ozone R ND ND
Paraffin wax R R R
Perchloric acid NR NR NR
Petroleum spirits R R R
Phenol NR NR NR
Phosphoric acid (20%) NR NR NR
Phosphoric acid (50%) NR NR NR
Phosphoric acid (95%) NR NR NR
Phosphorous chlorides ND ND ND
Phosphorous pentoxide R R ND
Phthalic acid R NR NR
Picric acid R NR NR
Pyridine R ND ND
Salicyl aldehyde ND ND ND
Sea water R R R
Silicic acid ND ND ND
Silicone fluids R ND ND
Silver nitrate R ND ND
Sodium carbonate R ND ND
Sodium peroxide NR NR NR
Sodium silicate R R R
Sodium sulphide R ND ND
Stannic chloride R ND ND
Starch R R R
Sugar, syrups & jams R R R
Sulphamic acid NR NR NR
Sulphates (Na, K, Mg, Ca) R R R
Sulphites ND ND ND
Sulphonic acids NR NR NR
Sulphur R ND ND
Sulphur dioxide, dry R ND ND
Sulphur dioxide, wet R NR NR
Sulphur dioxide (96%) NR NR NR
Sulphur trioxide NR NR NR
Sulphuric acid (<50%) NR NR NR
Sulphuric acid (70%) NR NR NR
Sulphuric acid (95%) NR NR NR
Sulphuric acid, fuming NR NR NR
Sulphur chlorides ND ND ND
Tallow R ND ND
Tannic acid (10%) R ND ND
Tartaric acid R R ND
Trichlorethylene R R R
Urea (30%) R R R
Vinegar R ND ND
Water, distilled. R R R
Water, soft R R NR
Water, hard R R R
Wetting agents (<5%) R R R
Yeast R ND ND
Zinc chloride NR NR NR

 